Qo'shma Shtatlar va Rossiyadagi asosiy yuqori quvvatli titanium qotishmalarining kimyoviy tarkibi va mexanik xususiyatlari
Qotishma turi | Qotishma darajasi | qotishma tarkibi | Mo ekvivalenti | Issiqlik bilan ishlov berish | a/MPa | d/ foiz |
ortiqcha qotishma | Ti-431 | Ti-4A1-3Mo-1V | 3.7 | Söndürme va qarish | 1350 | 3-5 |
BT14 | Ti-5A1-3Mo-1V | 3.7 | Söndürme va qarish tavlanish | 1275 1190 | 4-6 11.5 | |
Ti-62222S | Ti-6A1-2Sn-2Z--2Mo-2Cr-0.25Si | 5.3 | Söndürme va qarish tavlanish | 1330 1162 | 7.5 10 | |
Ti-6246 | Ti-6A1-2Sn-4Zr-6Mo | 6.0 | Söndürme va qarish Yuvish | 1214 1105 | 13 12 | |
BT3-1 | Ti-6A1-2.5Mo-1.5Cr-0.5Fc-0.3S | 6.0 | Söndürme va qarish Yuvish | 1270 1150 | 7-12 7 | |
BT23 | Ti-5A1-4.5V-2Mo-1Cr-0.6F | 8.1 | Söndürme va qarish Yuvish | 1460 1007 | 5 dan katta yoki teng 18.4 | |
SP-700 | Ti-45A1-3V-2Mo-2Fe | 8.1 | Söndürme va qarish Yuvish | 1377 890 | 12 14 dan katta yoki teng | |
BT16 | Ti-3A1-4,5V-5Oy | 8.2 | Söndürme va qarish | 1100 | 14 | |
Yaqin metastabil qotishmalar | BT22M | Ti-5AI-5M0-1V-1Cr-1Fe-1.5Sn-2Zr | 9.4 | tavlanish | 1200 | 6 dan katta yoki teng |
BCEZ | Ti-5A1-4Mo-2Cr-12Fe-2Sn-4Zr | 9.7 | Söndürme va qarish Yuvish | 1506 1160 | 13 10 | |
Ti-17 | Ti-5A1-2Sn-4Mo-4Cr-2Zr | 10.7 | Söndürme va qarish | 1300 | 13 | |
Ⅲ | Ti-11.5Mo-6Zr-4.5Sn | 11.5 | Söndürme va qarish | 1413 | 7 | |
Ti-1023 | Ti-10V-2Fe-3A1 | 11.1 | Söndürme va qarish tavlanish | 1275 1175 | 7.5 12 | |
BT22 | Ti-5A1-4,75Mo-4,75V-1Cr-1Fe | 11.8 | Söndürme va qarish | 1475 | 8 | |
Metastabil qotishmalar | BT22i | Ti-3A1-5V-5Mo-12Cr-1.2Fe | 13.0 | tavlanish | 1100 | 8 dan katta yoki teng |
Ti-2041 | Ti-4A1-20V-1Sn | 14.3 | Söndürme va qarish | 1530 | 6 | |
Ti-15-3 | Ti-15V-3A1-3Cr-3Sn | 15.7 | Söndürme va qarish | 1475 | 14 | |
B21S | Ti-15Mo-3A1-2.7Nb-0.25Si | 15.8 | Söndürme va qarish | 1260 | 4-5 | |
Timet LCB | Ti-6.8Mo-4.5Fe-1.5A1 | 15.8 | Söndürme va qarish | 1470 | 5-8 | |
BT35 | Ti-15V-3Cr-3Al-3Sn-1Zr-1Mo | 16.7 | Söndürme va qarish | 1275 | 8 dan katta yoki teng | |
Ti-8823 | Ti-8Mo-8V-2Fe-3Al | 17.7 | Söndürme va qarish | 1250 | 7-8 | |
BT32 | Ti-8V-8Mo-1.5Cr-1.5Fe-3Al | 19.2 | Söndürme va qarish | 1250 | 8 dan katta yoki teng | |
C | Ti-8V-6Cr-4Mo-4ZT-3AI | 19.7 | Söndürme va qarish | 1117 | 18 | |
Ti-13-11-3 | Ti-13V-11Cr-3AI | 27.6 | Söndürme va qarish | 1400 | 6-8 |